For site engineers, QC staff and ready-mix users in the UAE: enter the kg of cement, aggregate and water in 1 m³ of mix and their temperatures in °C, and get the fresh concrete temperature, a check against your maximum placing temperature, and the chilled water temperature needed to meet it.
Worked example
With the calculator’s starting values:
| Cement | 350 kg |
|---|---|
| Aggregates, saturated surface dry | 1,850 kg |
| Free water on the aggregates | 30 kg |
| Mixing water added | 160 kg |
| Cement temperature | 45 °C |
| Aggregate temperature | 35 °C |
| Mixing water temperature | 25 °C |
| Maximum placing temperature | 32 °C |
| Fresh concrete temperature | 33.8 °C |
|---|---|
| Against the limit | Above the limit |
| Maximum placing temperature | 32 °C |
| Mixing water temperature to meet the limit | 17.6 °C |
How it is calculated
T = [0.22 × (Ta × Wa + Tc × Wc) + Tw × Ww + Ta × Wwa] ÷ [0.22 × (Wa + Wc) + Ww + Wwa]
Water temperature for the limit = [Tmax × bottom term − 0.22 × (Ta × Wa + Tc × Wc) − Ta × Wwa] ÷ Ww
W = mass in kg per m³, T = temperature in °C; a = aggregate, c = cement, w = added water, wa = free water on the aggregate
About the formula
This is the standard heat balance for fresh concrete given in ACI 305R, Guide to Hot Weather Concreting. It uses 0.22 as the specific heat of cement and aggregate relative to water, and ignores heat from mixing and from early hydration, so the concrete at the pump can be a little warmer than the result.
Defaults you can change
The mix weights and temperatures are example values. Use your approved mix design and measured temperatures. The 32 °C limit is also an example; use the maximum placing temperature in your project specification. For admixtures and supplementary materials, add their weight to the cement if they are a large share of the binder.
Hot weather concreting in the UAE
Summer shade temperatures in the UAE often pass 40 °C, so aggregates stockpiled in the sun and hot cement can push fresh concrete above the specified placing temperature. Ready-mix plants serving Dubai, Sharjah, Abu Dhabi and Ajman commonly use chilled water or ice in summer, shade the aggregate, and many sites pour at night. Water has the biggest effect per kg, which is why cooling the mixing water is the first step.
Questions
Which material has the most effect on concrete temperature?
Aggregate, because it is most of the mix by weight. Water has the strongest effect per kg, so chilled water is the easiest control.
What if the result says the limit is not reachable with chilled water alone?
Even 0 °C water would not bring the mix down to the limit. Replace part of the water with ice, cool or shade the aggregate, or pour at a cooler time.
Is 32 °C the limit in the UAE?
It is only an example here. Use the limit in your project specification.