For painting contractors, coating inspectors and site engineers in the UAE: enter the target dry film thickness in microns, the volume solids and any thinner, and get the wet film thickness to check with a WFT comb, plus the litres for your area in m².
Worked example
With the calculator’s starting values:
| Target dry film thickness (DFT) | 100 µm |
|---|---|
| Volume solids | 50 % |
| Thinner added | 10 % |
| Area to coat | 100 m² |
| Number of coats | 1 nr |
| Loss allowance | 0 % |
| Wet film thickness to apply | 220 µm |
|---|---|
| WFT without thinner | 200 µm |
| Theoretical spreading rate | 5 m²/L |
| Paint needed (unthinned) | 20 L |
| Thinner needed | 2 L |
How it is calculated
WFT = DFT × 100 ÷ volume solids % × (1 + thinner %)
Theoretical spreading rate (m²/L) = volume solids % × 10 ÷ DFT (µm)
Paint needed = area × coats ÷ spreading rate × (1 + loss allowance)
Thinner needed = paint needed × thinner %
Thinner adds volume but evaporates, so a thinned coat must go on wetter to leave the same dry film. In the example, 100 µm dry at 50% volume solids needs 200 µm wet, and with 10% thinner it needs 220 µm wet.
Checking WFT on site
Press a wet film comb into the fresh coat straight away and read the last tooth that is wet. Check several spots and adjust the application. The dry film should still be confirmed with a DFT gauge once the coat has cured.
Defaults you can change
The DFT, volume solids, thinner and area are examples. Take the volume solids and allowed thinner from the product data sheet and the DFT from the specification. The theoretical spreading rate has no losses, so add your own loss allowance.
Coating thickness in the UAE
Specifications for steelwork, tanks and concrete coatings on projects in Dubai, Sharjah, Abu Dhabi and Ajman usually state a DFT for each coat, and inspectors check it. High temperatures make solvents evaporate faster, so read the wet film straight after application and follow the data sheet for thinning and application limits in hot weather.
Questions
What is the difference between WFT and DFT?
WFT is the thickness of the coat when it is applied. DFT is what is left after the solvent or water evaporates. Volume solids links the two.
Where do I find volume solids?
On the product data sheet, usually as a percentage by volume.
Does thinner change the DFT?
No. It raises the wet film you need for the same DFT, because the thinner evaporates.